Process for molding 107056-25-100
* Must use hot oil mold heater to heat both mold halves to 320 degrees
F.
* First stage injection time is 2.5 seconds at 750 PSI.
* Second stage holding time is 5 seconds at 400 PSI.
* Cure time must be 35 seconds minimum.
* Must have at least 35 seconds to ensure part transfer from A side to
B side
* Stock temperature:
* Rear zone 530 degrees F
* Middle zone 560 degrees F
* Front zone 570 degrees F
* Nozzle temperature 575 degrees F
* Material must dry for a minimum of 3 hours.
Additional notes: Mold temperature is very important. Cannot vary too much. Must make sure material is dry. Very important.